Product

AQUASHUTTER

Waterproof Flexible Cement Membrane

Description

2-component waterproofing cement

The product is a cement-based waterproofing material with two components (polymer cement), used in blending acrylic resin emulsions and special cementitious additives. Aquashutter is invented based on the technical formula of UBE Corporation and used for more than 20 years in Japan.

Product Details

ACG Emulsion – Emulsion for waterproofing:
ACG emulsion is a durable acrylic emulsion and used as waterproofing agent ( ACG material) after mixing with ACG admixture.

  • Packing content 18 kg/PP can.
  • Appearance: Milky white liquid.

ACG Admixture – Admixture for Waterproofing:
ACG admixture is a alumina cement based admixture and use as waterproofing agent (ACG material) mixing with ACG emulsion.

  • Packing Content: 15kg/ bag
  • Appearance: Gray powder

Properties

The material is similar to a Urethane coating, which is less susceptible to UV rays or hydrolysis.

In particular, Aquashutter has been highly weather-resistant, flexible elasticity, and waterproofing during a long period.

The product can be applied in waterproofing water tanks, underground interior, underground exterior, toilet, bathroom, kitchen, bathroom, trench pits, elevator pit.

Durability Test​

Technical report

Tensile strength

N/m2

1.1

Elongation

%

145

Zero span tension elongation

mm

3.9

Adhesion strength (dry)

N/mm2

0.8

Water Permeability

gram

0.1

Test condition

temperature

20±2℃

Humidity:

65±5%

Test method
Architectural Institute of Japan (Polymer-modified cement waterproofing membrane coating

Application method

1. Priming Paint:
    • Use ACG emulsion diluted 5 times in water. Blending ratio (weight ratio): ACG emulsion: water = 1:4
    • Primer with 0.2kg/m2 uniformly using a paint roller
2. Mixing Instruction:
Mixing ratio ACG emulsion: ACG admixture= 18: 30 [15 × 2 bags].
    1. Place the pure ACG Emulsion into the vessel.
    2. Combine the ACG mixture with manual mixer.
    3. Add two bags of ACG admixture to the above mixture.
    4. After 3 minutes of mixing, inspect to make sure there are no lumps.

Batching Process

3. Waterproof Coating (ACG material) – First Coat, Top Coat
    1. Use a steel trout to apply the waterproofing coat to the surface and then smooth the coated sealant. Note: Use hand force when handling to help the waterproof layer increase adhesion.
    2. The quantity of paint used in construction is 1.2 kg / m2 (once only).
After making sure it has hardened so that it does not leave fingerprints when pressed, apply a second coat.
  • Verify that the pinhole on the first coat is dry before applying the second coat.
  • In case of pinhole appearance, fill with ACG material and proceed with the second coat until there is no pinhole of the first coat.
4. Maintenance:
  1. Use a fan or similar device to adequately ventilate the waterproofing surface to prevent condensation.
  2. If rain is forecast, construction must be shut down. If the waterproof coat is washed out by rain after application, the coating must be redone.

other Products

cerinol_z4448074171964_da162a66b7e9096f4f3dcf7e016278cd
CERINOL DS
Waterproof Osmotic Cement
z4484045830418_267783b53d40a3f5d24718f4bf8d1515
AQUAMENT
Polymer-modified cementitious waterproofing membrane coating
tap_grout_z4448085101467_caff980c71ad88ec563b8e6efe26bafd
TAP GROUT
High-pressure Spraying Method for Preventing Water Leakage

Contact Us

We look forwards to collaborating with your company. Please fill in your information, we will contact at your earliest convenience.

    Vui lòng chọn vấn đề bạn cần hỗ trợ / Please select: